Independent welding consumables professional
- FMA
- The Fabricator
- FABTECH
- Canadian Metalworking
Categories
- Additive Manufacturing
- Aluminum Welding
- Arc Welding
- Assembly and Joining
- Automation and Robotics
- Bending and Forming
- Consumables
- Cutting and Weld Prep
- Electric Vehicles
- En Español
- Finishing
- Hydroforming
- Laser Cutting
- Laser Welding
- Machining
- Manufacturing Software
- Materials Handling
- Metals/Materials
- Oxyfuel Cutting
- Plasma Cutting
- Power Tools
- Punching and Other Holemaking
- Roll Forming
- Safety
- Sawing
- Shearing
- Shop Management
- Testing and Measuring
- Tube and Pipe Fabrication
- Tube and Pipe Production
- Waterjet Cutting
Industry Directory
Webcasts
Podcasts
FAB 40
Advertise
Subscribe
Account Login
Search
Consumables Corner: Identifying pockmarking causes in structural SAW
- By Nino Mascalco
- June 16, 2014
- Article
- Consumables
Q: Our company manufactures various structural components, typically made from A36 or A572 steel grades in plate, I-beam, or channel. Based on the application we’ll use GMAW, FCAW, or SAW. On random occasions we experience pockmarking on the surface of the SAW joints. While the timing is usually unpredictable, we’ve found that it typically shows up on horizontal fillet (2F) T-joint welds or on the cover pass of exterior weld joints of rolled plate components. I understand that this issue is not considered a weld defect, but the appearance is not desirable. Is there a remedy for this?
A: There are several explanations for the pockmarking you are experiencing. For starters, if this problem began happening fairly recently, you may want to revisit any news process, consumable, or material changes. It's not uncommon for companies nowadays to make changes that might appear insignificant to the manufacturing processes in an effort to run lean. Sometimes, however, these changes end up having unforeseen effects.
Assuming you have approved weld procedures, make sure your welders are following them closely. Excessive electrical stick-out (ESO) has been known to cause a similar weld surface issue. Additionally, most flux-delivery nozzles are attached directly to the welding torch and if the ESO is excessive, the amount of flux burden may be too deep. This could lead to improper degassing of the molten weld puddle.
Pockmarking also may be caused by an improper ratio of recycled-to-virgin flux or by lack of flux-recovery system cleaning. Every time you recycle flux, the particles tend to break down into smaller mesh sizes. This could allow too many flux fines to accumulate in the system, which also prohibits proper degassing of the weld puddle during the welding process.
A more common culprit of pockmarking is excessive moisture in the flux. Proper intermediate- and long-term storage of flux is essential. That information is supplied by your flux manufacturer, but typically keeping the flux temperature above the boiling point of water (212 degrees F or 100 degrees C) should prevent any moisture buildup.
Without knowing your complete history and assuming you have always had issues with pockmarking, the next thing to consider is welding process variables. How well are your ESO, voltage, current, and travel speed controlled? How is the flux delivered to the joint, and what is the flux burden depth? What is the ratio of recycled flux to virgin flux, and how often is the flux-recovery system cleaned? Is your flux stored in a heated holding tank, and if so, what is the temperature? Is the material surface clean? Is there any oil, rust, or mill scale in the welding joint area? If the flux delivery is through an air pressure hose, make sure the air is dry and clean (no oil).
Each one of these items can play a significant role in weld performance. If more than one variable is out of the recommended range, they may combine to cause welding issues that also make determining the root cause more challenging.
About the Author
About the Publication
Related Companies
subscribe now
The Welder, formerly known as Practical Welding Today, is a showcase of the real people who make the products we use and work with every day. This magazine has served the welding community in North America well for more than 20 years.
start your free subscription- Stay connected from anywhere
Easily access valuable industry resources now with full access to the digital edition of The Fabricator.
Easily access valuable industry resources now with full access to the digital edition of The Welder.
Easily access valuable industry resources now with full access to the digital edition of The Tube and Pipe Journal.
Easily access valuable industry resources now with full access to the digital edition of The Fabricator en Español.
- Podcasting
- Podcast:
- The Fabricator Podcast
- Published:
- 05/14/2024
- Running Time:
- 62:12
Cameron Adams of Laser Precision, a contract metal fabricator in the Chicago area, joins the podcast to talk...
- Trending Articles
Connecticut students compete in Maritime Welding Competition
Welding power source’s modes designed to help optimize performance
Building a successful welding program from the ground up
Torch made for welding thin, conductive sheet metal
Welding jacket designed for protection, comfort
- Industry Events
Laser Welding Certificate Course
- May 7 - August 6, 2024
- Farmington Hills, IL
World-Class Roll Forming Workshop
- June 5 - 6, 2024
- Louisville, KY
Advanced Laser Application Workshop
- June 25 - 27, 2024
- Novi, MI
Precision Press Brake Certificate Course
- July 31 - August 1, 2024
- Elgin,