Project Engineer
- FMA
- The Fabricator
- FABTECH
- Canadian Metalworking
Categories
- Additive Manufacturing
- Aluminum Welding
- Arc Welding
- Assembly and Joining
- Automation and Robotics
- Bending and Forming
- Consumables
- Cutting and Weld Prep
- Electric Vehicles
- En Español
- Finishing
- Hydroforming
- Laser Cutting
- Laser Welding
- Machining
- Manufacturing Software
- Materials Handling
- Metals/Materials
- Oxyfuel Cutting
- Plasma Cutting
- Power Tools
- Punching and Other Holemaking
- Roll Forming
- Safety
- Sawing
- Shearing
- Shop Management
- Testing and Measuring
- Tube and Pipe Fabrication
- Tube and Pipe Production
- Waterjet Cutting
Industry Directory
Webcasts
Podcasts
FAB 40
Advertise
Subscribe
Account Login
Search
Tube Hydroforming Design Flexibility—Part VI
- By Gary Morphy
- September 14, 2004
- Article
- Hydroforming
Forming Corners
In expansion, the cross-section corner radius is an important consideration. As increased pressure stretches material into the corners, it also stretches the metal that is not yet in contact with the die surface, as shown in Figure 1. The stretched material decreases in width and becomes progressively thinner near where the wall is tangent to the die. This effect is more noticeable in sharper corners. Making the cross-sectional corner radius larger decreases the likelihood of rupture.
Figure 1 |
When the part is not being expanded, such as with pressure sequence hydroforming (PSH), the cross section forms as shown in Figure 2. This is a fundamentally different forming mechanism from that shown in Figure 1. Since water pressure is in the tube while the die is closing, it is the action of the die that causes the corners to form rather than the forming fluid, as is the case in Figure 1. Figure 2 shows compressive forces pushing the wall into the cross-sectional corner. As a result, the radius formed is not dependent on the water pressure being used.
Figure 2 |
Corner sharpness often is expressed as a multiple of the wall thickness— a common practice in the stamping industry. As can be seen in Figure 3, sharp corners relative to wall thickness can be achieved in a production part. The wall thickness shown is approximately 1.2 mm, and the outside corner radius is as small as 3.5 mm.
Figure 3 |
This factor is a key determinant of the maximum pressure required to completely form a part using high-pressure hydroforming (HPH) after the structural demands of material yield strength (YS) and thickness have been satisfied (Equation 1).
Equation 1 |
Using HPH to produce sharper corners, which increases internal pressure in cross sections, can be expensive. The pressure-generation equipment, the hydraulic process, and the hydroforming tool all must be proportionately stronger to achieve the desired corner. Increased die wear and selecting the right lubricant and material formable enough to prevent rupture also can increase cost.
Because corner sharpness does not depend on pressure with PSH, using this process to design sharper corners normally does not change the forming pressure or inflate costs. Furthermore, because PSH does not thin material in the corners and because the residual stresses are compressive rather than tensile, rupturing is not a concern.
Several design considerations favor sharper corners. One is extending flat surfaces for welding or placing a hole near a corner. Structurally, sharper corners improve a section's rigidity. Sharpening the corners is a technique that can be used to make parts more compact to accommodate packaging restrictions in the vehicle. A less tangible reason for making the corners sharper is that the part looks sharper and better defined—of higher quality.
Figure | Material Grade (SAE No.) | Min. Wall Thickness (T) mm | Internal Pressure (MPa) | Outside Corner Radius | Yield Stress (MPa) |
4 | 1010 | 2.0 | 37.2 | 4.75T | 263 |
5 | 1010 | 3.0 | 37.2 | 3.2T | 296 |
1026 | 6.3 | 41.4 | 1.5T | 386 |
Table 1 |
Figures 4 and 5 and Table 1 illustrate that internal pressure used in the PSH process is not sensitive to corner sharpness. Corner sharpness can decrease 30 percent with no effect at all. Even a decrease of 70 percent generates only a 10 percent pressure increase. It is likely that even this P increase was unnecessary, but the experimental forming did not confirm this.
Part Features (Forming Severity)
HPH techniques are well-suited to bulge forming as evidenced by many prototype parts that have been publicized. Examples are plumbing fittings, in particular T's, bicycle frame nodes, and camshafts.
Protrusions like those found on these parts would seem to be beneficial on automotive structural parts. It is unclear if their inclusion is technically or economically feasible in larger, normally steel structural parts. Several designs that included them evolved into production designs, in which they disappeared.
Indents that cannot be formed with a solid portion of the die can be accomplished by moving a portion of the cavity wall after the die is closed. Features that would create a die lock condition are an example. It probably is best to form such features when internal pressure is highest, but because this increases the size of the actuator needed, it is best to determine the lowest pressure needed for proper forming. Actuation units must be proportionately larger with HPH (because max. pressure is much higher than with PSH), with possible limitations on in-die hole punching or die integrity. Similarly, cross-section corners can be made sharper with such a mechanism.
PSH is better-suited to forming sharp corners, punching large numbers of holes, and creating dramatic indents, because the pressure used is much lower. High-strength materials as well as those with lower elongation can be formed with the same fluid pressure and press size used for lower-strength metals.
About the Author
Gary Morphy
425 Hespeler Rd Suite 521
Cambridge, ON N1R 8J6 Canada
(519) 772 - 5748 x101
About the Publication
Related Companies
subscribe now
The Tube and Pipe Journal became the first magazine dedicated to serving the metal tube and pipe industry in 1990. Today, it remains the only North American publication devoted to this industry, and it has become the most trusted source of information for tube and pipe professionals.
start your free subscription- Stay connected from anywhere
Easily access valuable industry resources now with full access to the digital edition of The Fabricator.
Easily access valuable industry resources now with full access to the digital edition of The Welder.
Easily access valuable industry resources now with full access to the digital edition of The Tube and Pipe Journal.
Easily access valuable industry resources now with full access to the digital edition of The Fabricator en Español.
- Podcasting
- Podcast:
- The Fabricator Podcast
- Published:
- 05/07/2024
- Running Time:
- 67:38
Patrick Brunken, VP of Addison Machine Engineering, joins The Fabricator Podcast to talk about the tube and pipe...
- Trending Articles
Zekelman Industries to invest $120 million in Arkansas expansion
Making the move from hard automation to robotic welding
Brushless copper tubing cutter adjusts to ODs up to 2-1/8 in.
HGG Profiling Equipment names area sales manager
Miscellaneous metals fabricator increases productivity and opportunity with plasma cutting
- Industry Events
Laser Welding Certificate Course
- May 7 - August 6, 2024
- Farmington Hills, IL
World-Class Roll Forming Workshop
- June 5 - 6, 2024
- Louisville, KY
Advanced Laser Application Workshop
- June 25 - 27, 2024
- Novi, MI
Precision Press Brake Certificate Course
- July 31 - August 1, 2024
- Elgin,